Non-destructive testing does not make the pipe better. It reports what was found, on the items tested, under the procedure used. UT, RT, MT and PT are sensitive to different defect types in different places, so the method has to be chosen against the defect the pipe standard is trying to exclude.
What each method is sensitive to
| Method | Sensitive to | Where | Limit to remember |
|---|---|---|---|
| Ultrasonic testing (UT) | Planar defects such as cracks, laminations and lack of fusion | Internal and surface-connected | Needs a couplant, a calibration reference and a trained operator |
| Radiographic testing (RT) | Volumetric defects such as porosity and slag | Through the wall, as an image | Radiation safety controls; a tight planar crack can be missed |
| Magnetic particle testing (MT) | Surface and near-surface linear defects | Ferromagnetic material only | Does not apply to austenitic stainless steel |
| Dye penetrant testing (PT) | Defects open to the surface | Any non-porous material | Subsurface defects are not detected |
Ultrasonic testing
UT sends high-frequency sound into the wall and reads the reflected signal. It is the usual method for laminations in the raw material and for the weld seam, and it is also used to measure the wall. Thickness readings are normally reported to 0.1 mm, but the acceptance limit is the one in the pipe standard, not the resolution of the instrument. Calibration against a reference standard is part of the procedure.
Radiographic testing
RT produces an image of the wall on film or on a digital detector. It shows volumetric features well. It carries radiation safety obligations, including controlled access and personnel dosimetry, so it is scheduled rather than run continuously beside a production line.
Magnetic particle testing
MT magnetises the part and applies fine particles that gather at the leakage field of a discontinuity. It is fast on ferromagnetic material. It cannot be used on austenitic stainless steel or on other non-ferromagnetic alloys.
Dye penetrant testing
PT draws a penetrant back out of a surface opening with a developer. It is the surface method for non-magnetic material and for complex geometry. It only finds defects that are open to the surface.
What the pipe standard requires
The extent of testing is set by the specification and by the purchase order. API 5L requires non-destructive inspection of the weld seam for welded pipe, and PSL 2 adds requirements that PSL 1 does not carry. ASTM A106 does not mandate NDT as a default, so extra testing is a supplementary requirement the buyer has to name. Read the clause in the edition named on the order.
Published pipe pages that commonly carry these requirements include seamless carbon steel pipe, API 5L Grade B seamless pipe and 304 stainless steel seamless pipe. The grade does not select the method. The specification does.
What the report has to show
- The method, the procedure reference and the calibration standard used.
- The extent: seam only, full body, or the percentage and which items were covered.
- Identification of the pipes or heats tested, not only a batch reference.
- The acceptance criterion from the standard, and the result against it.
- Operator qualification where the specification requires it.
What to Confirm with Your Inquiry
- Pipe standard, edition, grade, and seamless or welded route.
- Which method is required, and on the seam, the body or the ends.
- Extent of examination and the acceptance criterion.
- Whether a third-party witness is required, and who carries the cost.
- How the report is identified to the heat and to the shipped lengths.
Method selection is a specification decision. For the wall the examination is applied to, see how to read a pipe wall-thickness schedule.