Product Description
Seamless stainless steel heat exchanger tubes supplied to ASTM A213, the specification for seamless ferritic and austenitic steel boiler, superheater and heat-exchanger tubes; the same document is carried into ASME BPVC Section II as SA-213. Tubes are made by the seamless process, hot-finished or cold-finished, and the austenitic grades are furnished in the heat-treated condition. The grades quoted on this page are TP304, TP304L, TP316 and TP316L, with H-grades handled on enquiry; the exact grade is confirmed for every order. For pipe ordered by nominal size and schedule, see the stainless steel pipe range instead.
Ordering Specification and Size Scope
The size scope in the table follows the wording of ASTM A213 on the sizes usually furnished to the specification, so enquiry dimensions can be checked against it before quotation.
| Ordering item | Range or basis |
|---|---|
| Size scope | 1/8 in. (3.2 mm) inside diameter to 5 in. (127 mm) outside diameter, as usually furnished to ASTM A213 |
| Wall thickness | 0.015 to 0.500 in. (0.4 to 12.7 mm), minimum-wall or average-wall basis stated on the order |
| Manufacturing route | Seamless, hot-finished or cold-finished as specified |
| Delivery condition | Solution annealed for the austenitic grades in this range |
| Length | Random or fixed lengths; the requested length is confirmed with the quotation |
Tubing outside these diameters can be furnished when it complies with all other ASTM A213 requirements; send the drawing with the enquiry for confirmation.
Chemical Composition of the Name Grades
The ladle-analysis limits below are the ASTM A213 composition requirements for TP304 and TP316L, the two grades named on this page; the edition stated on the purchase order governs the full analysis.
| Grade | UNS | C, max % | Mn, max % | Cr, % | Ni, % | Mo, % |
|---|---|---|---|---|---|---|
| TP304 | S30400 | 0.08 | 2.00 | 18.0–20.0 | 8.0–11.0 | – |
| TP316L | S31603 | 0.035 | 2.00 | 16.0–18.0 | 10.0–14.0 | 2.00–3.00 |
TP304L and TP316L are the low-carbon variants, with the carbon maximum reduced to limit sensitization in welded construction. Grades with an H suffix, such as TP304H and TP316H, carry separate requirements that provide higher creep-rupture strength in high-temperature service.
Mechanical Requirements, Solution Annealed
The minimum room-temperature properties in the table are the ASTM A213 tension-test requirements for the four grades quoted on this page in the solution-annealed condition.
| Grade | Tensile strength, min | Yield strength, min | Elongation in 2 in. or 50 mm, min | Hardness, max |
|---|---|---|---|---|
| TP304 | 515 MPa (75 ksi) | 205 MPa (30 ksi) | 35 % | 90 HRB |
| TP304L | 485 MPa (70 ksi) | 170 MPa (25 ksi) | 35 % | 90 HRB |
| TP316 | 515 MPa (75 ksi) | 205 MPa (30 ksi) | 35 % | 90 HRB |
| TP316L | 485 MPa (70 ksi) | 170 MPa (25 ksi) | 35 % | 90 HRB |
For cold-finished tubes, typical outside-diameter tolerances are ±0.10 mm below 25.4 mm OD, ±0.15 mm for 25.4 to 38.1 mm and ±0.20 mm for 38.1 mm to below 50.8 mm. Minimum-wall tubing carries a +20 % over-tolerance with no minus tolerance up to 38.1 mm OD, and +22 % above that size. The tolerances printed on the ordered edition, together with ASTM A1016 where applicable, govern the final inspection.
Heat Treatment and Product Testing
Austenitic tubes under ASTM A213 are furnished in the heat-treated condition: solution annealed at 1040 °C (1900 °F) minimum and rapidly cooled so carbides remain in solution. Each tube is then tested to the specification: tension, hardness, flattening and flaring tests, followed by a nondestructive electric test or a hydrostatic test of every tube. Material test certificates, intergranular-corrosion testing and positive material identification can be arranged with the order; state the required documentation when you send the enquiry.
Where These Heat Exchanger Tubes Are Used
Typical service includes shell-and-tube heat exchangers, boilers, superheaters, reheaters, feedwater heaters and condensers in power generation, petrochemical and chemical processing plants, and steam generators where austenitic stainless construction is specified. Grade selection follows the corrosion and temperature requirements of the design: TP304 for general service, and TP316L where the molybdenum-bearing composition and lower carbon maximum are required for welded, chloride-exposed duty.
Ordering Information
Include the following inputs with your enquiry so the quotation can be checked against the specification:
- ASTM A213 with the edition, and the exact grade including L or H suffix.
- Outside diameter, wall thickness and the wall basis (minimum or average).
- Length, quantity and any equipment drawing or datasheet.
- Delivery condition, surface finish and additional processing such as U-bending.
- Inspection scope, certificates and destination.
Questions Before You Order
Do you supply ASTM A213 tubes in SCH 10, SCH 40 or SCH 80?
Schedule numbers such as SCH 10, SCH 40 and SCH 80 are pipe designations, not heat-exchanger tube sizes; ASTM A213 tube is ordered by actual outside diameter and wall thickness on a minimum-wall or average-wall basis. If the enquiry also covers pipe, see the seamless and welded stainless steel pipe in SCH 10 to SCH 80.
Should I order TP304 or TP316L for my heat exchanger?
Use the grade stated on the mechanical design or purchasing specification. TP304 is the general-purpose composition; TP316L adds 2.00–3.00 % molybdenum and lowers the carbon maximum to 0.035 % for welded, chloride-exposed service. The grades are separate selections, not interchangeable, and the exact grade is confirmed for every order.
What is the difference between minimum wall and average wall?
ASTM A213 accepts either basis when it is stated on the order. Minimum-wall tubing carries a +20 % over-tolerance with no minus tolerance up to 38.1 mm outside diameter, while average-wall tubing applies tolerances on both sides of the nominal wall. State the basis used in your calculation so inspection and certification match the design.
What are TP304H and TP316H?
Grades with an H suffix have different requirements under ASTM A213 that provide higher creep-rupture strength for high-temperature service such as superheaters and reheaters. If your datasheet calls for an H-grade, send it with the outside diameter, wall and length so availability is confirmed with the quotation.